SVENSK STANDARD SS-EN 1011-3
Fastställd 2001-05-18 Utgåva 1
ICS 25.160.10 Språk: engelska, svenska Tryckt i december 2002
© Copyright SIS. Reproduction in any form without permission is prohibited.
Svetsning – Rekommendationer för svetsning av metalliska material –
Del 3: Bågsvetsning av rostfritt stål
Welding – Recommendations for welding of metallic materials –
Part 3: Arc welding of stainless steels
Dokumentet består av 62 sidor.
Upplysningar om sakinnehållet i standarden lämnas av SIS, Swedish Standards Institute, tel 08 - 555 520 00.
Standarder kan beställas hos SIS Förlag AB som även lämnar allmänna upplysningar om svensk och utländsk standard.
Postadress: SIS Förlag AB, 118 80 STOCKHOLM Telefon: 08 - 555 523 10. Telefax: 08 - 555 523 11 E-post: sis.sales@sis.se. Internet: www.sis.se
Europastandarden EN 1011-3:2000 gäller som svensk standard. Europastandarden fastställdes 2001-05-18 som SS-EN 1011-3 och har utgivits i engelsk språkversion. Detta dokument, som ersätter det tidigare, åter- ger EN 1011-3:2000 i tvåspråkig version.
Denna standard har utarbetats i samarbete med Svetskommissionen.
The European Standard EN 1011-3:2000 has the status of a Swedish Standard. The European Standard was 2001-05-18 approved and published as SS-EN 1011-3 in English. This document contains a bilingual version that supersedes the English version.
This standard has been developed in collaboration with the Swedish Welding Commission.
EUROPEAN STANDARD NORME EUROPÉENNE EUROPÄISCHE NORM
EN 1011-3
September 2000
ICS 25.160.10
English version
Welding - Recommendations for welding of metallic materials - Part 3: Arc welding of stainless steels
Soudage - Recommandations pour le soudage des matériaux métalliques - Partie 3: Soudage à l'arc des aciers
inoxydables
Schweißen - Empfehlungen zum Schweißen metallischer Werkstoffe - Teil 3: Lichtbogenschweißen von
nichtrostenden Stählen
This European Standard was approved by CEN on 13 August 2000.
CEN members are bound to comply with the CEN/CENELEC Internal Regulations which stipulate the conditions for giving this European Standard the status of a national standard without any alteration. Up-to-date lists and bibliographical references concerning such national standards may be obtained on application to the Central Secretariat or to any CEN member.
This European Standard exists in three official versions (English, French, German). A version in any other language made by translation under the responsibility of a CEN member into its own language and notified to the Central Secretariat has the same status as the official versions.
CEN members are the national standards bodies of Austria, Belgium, Czech Republic, Denmark, Finland, France, Germany, Greece, Iceland, Ireland, Italy, Luxembourg, Netherlands, Norway, Portugal, Spain, Sweden, Switzerland and United Kingdom.
EUROPEAN COMMITTEE FOR STANDARDIZATION C O M I T É E U R O P É E N D E N O R M A L I S A T I O N E U R O P Ä I S C H E S K O M I T E E F Ü R N O R M U N G
Central Secretariat: rue de Stassart, 36 B-1050 Brussels
© 2000 CEN All rights of exploitation in any form and by any means reserved worldwide for CEN national Members.
Ref. No. EN 1011-3:2000 E
EUROPASTANDARD EUROPEAN STANDARD NORME EUROPÉENNE EUROPÄISCHE NORM
EN 1011-3
September 2000
ICS 25.160.10
CEN
European Committee for Standardization Comité Européen de Normalisation Europäisches Komitee für Normung
Central Secretariat: rue de Stassart 36, B-1050 BRUSSELS
© 2000 CEN All rights of exploitation in any form and by any means reserved worldwide for CEN national Members
Ref. Nr. EN 1011-3:2000 Sv
Svensk version
Svetsning – Rekommendationer för svetsning av metalliska material – Del 3: Bågsvetsning av rostfritt stål
Soudage – Recommendations pour le soudage des matériaux
métalliques – Partie 3: Soudage à l’arc des aciers inoxydables
Welding – Recommendations for welding of metallic materials – Part 3: Arc welding of stainless steels
Schweißen – Empfehlungen zum Schweißen metallischer Werkstoffe – Teil 3: Lichtbogenschweißen von nichtrostenden Stählen
Denna standard är den officiella svenska versionen av EN 1011-3:2000. För översättningen svarar SIS.
Denna europastandard antogs av CEN den 13 augusti 2000.
CEN-medlemmarna är förpliktade att följa fordringarna i CEN/CENELECs interna bestämmelser som anger på vilka villkor denna europastandard i oförändrat skick skall ges status som nationell standard. Aktuella förteckningar och bibliografiska referenser rörande sådana nationella standarder kan på begäran erhållas från CENs centralsekretariat eller från någon av CENs medlemmar.
Denna europastandard finns i tre officiella versioner (engelsk, fransk och tysk).
En version på något annat språk, översatt under ansvar av en CEN-medlem till sitt eget språk och anmäld till CENs centralsekretariat, har samma status som de officiella versionerna.
CENs medlemmar är de nationella standardiseringsorganen i Belgien, Danmark, Finland, Frankrike, Grekland, Irland, Island, Italien, Luxemburg, Nederländerna, Norge, Portugal, Schweiz, Spanien, Storbritannien, Sverige, Tjeckien, Tyskland och Österrike.
Page 2
EN 1011-3:2000
Contents Page
Foreword 3
Introduction 4
1 Scope 4
2 Normative references 4
3 Terms and definitions 5
4 Parent metal 6
5 Storage and handling 6
6 Welding consumables 6
7 Fabrication 7
8 Quality requirements of welds 9
9 Distortion 9
10 Post-weld cleaning 10
Annex A (informative) Welding of austenitic stainless steels 11 Annex B (informative) Welding of ferritic stainless steels 18 Annex C (informative) Welding of austenitic-ferritic stainless steels 22 Annex D (informative) Welding of martensitic and martensitic-austenitic
stainless steels 27
Annex ZA (informative) Clauses of this European Standard addressing
essential requirements or other provisions of EU Directives 30
Sida 2 EN 1011-3:2000
Innehåll
Sida
Förord ... 3
Orientering ... 4
1 Omfattning ... 4
2 Normativa hänvisningar ... 4
3 Termer och definitioner ... 5
4 Grundmaterial ... 6
5 Lagring och hantering ... 6
6 Svetstillsatsmaterial ... 6
7 Tillverkning ... 7
8 Kvalitetskrav för svetsar ... 9
9 Formförändringar ... 9
10 Rengöring efter svetsning ... 10
Bilaga A (informativ) Svetsning av austenitiska rostfria stål ... 11
Annex B (informativ) Svetsning av ferritiska rostfria stål ... 18
Bilaga C (informativ) Svetsning av austenít-ferritiska rostfria stål ... 22
Bilaga D (informativ) Svetsning av martensitiska och martensit-austenitiska rostfria stål ... 27
Bilaga ZA (informativ) Avsnitt i denna europastandard som behandlar grundläggande krav eller andra bestämmelser i EU-direktiv ... 30
Page 3
EN 1011-3:2000
Foreword
This European Standard has been prepared by Technical Committee CEN/TC 121
"Welding", the secretariat of which is held by DS.
This European Standard shall be given the status of a national standard, either by publication of an identical text or by endorsement, at the latest by March 2001, and conflicting national standards shall be withdrawn at the latest by March 2001.
This European Standard has been prepared under a mandate given to CEN by the European Commission and the European Free Trade Association, and supports essential requirements of EU Directive(s).
For relationship with EU Directive(s), see informative Annex ZA, which is an integral part of this standard.
According to the CEN/CENELEC Internal Regulations, the national standards organizations of the following countries are bound to implement this European Standard: Austria, Belgium, Czech Republic, Denmark, Finland, France, Germany, Greece, Iceland, Ireland, Italy, Luxembourg, Netherlands, Norway, Portugal, Spain, Sweden, Switzerland and the United Kingdom.
This European Standard is composed of the following parts:
Part 1: General guidance for arc welding Part 2: Arc welding of ferritic steels Part 3: Arc welding of stainless steels
Part 4: Arc welding of aluminium and aluminium alloys
Annexes A, B, C and D are informative.
Sida 3 EN 1011-3:2000
Förord
Denna europastandard har utarbetats av den tekniska kommittén CEN/TC 121 ”Welding” med sekretariat vid DS.
Denna europastandard skall ges status av nationell standard, antingen genom publicering av en identisk text eller genom ikraftsättning senast mars 2001, och motstridande nationella standarder skall upphävas senast mars 2001.
Standarden har utarbetats under ett mandat till CEN från EU och EFTA och stöder väsentliga fordringar i EU-direktiv.
Sambandet med EU-direktiv beskrivs i bilaga ZA, som ingår som en informativ del i denna standard.
Enligt CEN/s interna bestämmelser är standardiseringsorganen i följande länder förpliktade att införa denna standard: Belgien, Danmark, Finland, Frankrike, Grekland, Irland, Island, Italien, Luxenburg, Nederländerna, Norge, Portugal, Schweiz, Spanien, Storbritannien, Sverige, Tjeckien, tyskland och Österrike.
Denna europastandard består av följande delar:
Del 1: Allmänna riktlinjer för bågsvetsning Del 2: Bågsvetsning av ferritiska stål Del 3: Bågsvetsning av rostfritt stål
Del 4: Bågsvetsning av aluminium och aluminiumlegeringar.
Bilagorna A, B, C, och D är informativa.
Page 4
EN 1011-3:2000
Introduction
This European Standard is being issued with several annexes in order that it may be extended to cover the different types of steel which will be produced to all the European steel standards for stainless steels.
When this standard is referenced for contractual purposes, the ordering authority should state the need for compliance with the standard and such other annexes as are appropriate.
This standard gives general guidance for the satisfactory production and control of welding and details the possible detrimental phenomena which may occur with advice on methods by which they may be avoided. It is generally applicable to all stainless steels and is appropriate regardless of the type of fabrication involved, although the application standard may have additional requirements. Permissible design stresses in welds, methods of testing and acceptance levels are not included because they depend on the service conditions of the fabrication. These details should be obtained from the design specification.
This Part of this European Standard contains additional details for fusion welding of stainless steels and should be read in conjunction with the general recommendations in EN 1011-1.
1 Scope
This European Standard gives general recommendations for the fusion welding of stainless steels. Specific details relevant to austenitic, austenitic-ferritic, ferritic and martensitic stainless steels are given in annexes A to D.
2 Normative references
This European Standard incorporates by dated and undated reference, provisions from other publications. These normative references are cited at the appropriate places in the text and the publications are listed hereafter. For dated references, subsequent amendments to or revisions of any of these publications apply to this European Standard only when incorporated in it by amendment or revision. For undated references the latest edition of the publication referred to applies (including amendments).
EN 288-2 Specification and approval of welding procedures for metallic materials – Part 2: Welding procedure specification for arc welding
EN 439 Welding consumables - Shielding gases for arc welding and cutting
Sida 4 EN 1011-3:2000
Orientering
Denna europastandard utges i flera delar så att den kan utvidgas till att omfatta de olika typer av stål som produceras enligt alla europastandarder för rostfritt stål.
Vid hänvisning till denna standard för kontraktsändamål bör den beställande parten anföra behovet av överens- stämmelse med relevanta delar av denna standard och andra tillämpliga bilagor.
Denna standard ger allmänna riktlinjer för en tillfredsställande svetsproduktion och dess styrning av svets- ning och anger i detalj några av de skadliga fenomen som kan uppträda och med råd om metoder för att undvika dem. Den kan allmänt tillämpas på smältsvetsning av rostfritt stål och är lämplig oberoende av typen av berörd tillverkning, även om den relevanta tillämpningsstandarden kan ha ytterligare fordringar. Tillåtna dimensionerande spänningar, provningsmetoder och acceptansnivåer ingår inte i denna standard eftersom de är beroende av tillverkningsvillkoren. Dessa detaljer bör hämtas från konstruktionshandlingarna.
Denna del av denna europastandard innehåller tillägg för smältsvetsning av rostfritt stål och bör läsas till- sammans med den allmänna delen i EN 1011-1.
1 Omfattning
Denna europastandard ger allmänna rekommendationer för smältsvetsning av rostfritt stål.
Speciella upplysningar relevanta för austenitiska, austenit-ferritiska, ferritiska och martensitiska rostfria stål ges i bilagorna A till D.
2 Normativa hänvisningar
Denna europastandard inkorporerar genom daterade eller odaterade hänvisningar bestämmelser från andra nedan förtecknade publikationer. Dessa normativa hänvisningar på de platser i texten där bestämmelserna skall tillämpas. För daterade hänvisningar gäller senare publicerade tillägg, ändringar eller reviderade utgå- vor vid användning av denna europastandard endast när de har inkorporerats i denna genom tillägg, ändring eller reviderad utgåva. För odaterade hänvisningar gäller den senaste utgåvan (inklusive tillägg).
SS-EN 288-2 Specifikation för godkännande av svetsprocedurer för svetsning av metalliska material – Del 2: Svetsdatablad för bågsvetsning
SS-EN 439 Tillsatsmaterial för svetsning – Skyddsgaser för svetsning och skärning